Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VICTREX® PEEK 450G903 BLACK - PEEK - Victrex plc

Material Data Center offers the following functions for VICTREX® PEEK 450G903 BLACK:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Victrex PEEK datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
加工/物理特性价值单位Test Standard
ISO数据
模塑收缩率, 平行 0.9 % ISO 294-4, 2577
模塑收缩率, 垂直 1.3 % ISO 294-4, 2577
熔体 0.29 W/(m K) -
机械性能价值单位Test Standard
ISO数据
拉伸模量 3900 MPa ISO 527
屈服应力 98 MPa ISO 527
断裂伸长率 30 % ISO 527
弯曲模量, 23°C 3800 MPa ISO 178
Izod冲击强度, +23°C N kJ/m² ISO 180/1U
悬臂梁缺口冲击强度, +23°C 7 kJ/m² ISO 180/1A
肖氏硬度D 84.5 - ISO 7619-1
热性能价值单位Test Standard
ISO数据
熔融温度, 10°C/min 343 °C ISO 11357-1/-3
玻璃化转变温度, 10°C/min 143 °C ISO 11357-1/-2
热变形温度, 1.80 MPa 152 °C ISO 75-1/-2
线性热膨胀系数, 平行 45 E-6/K ISO 11359-1/-2
燃烧性-氧指数 35 % ISO 4589-1/-2
灼热丝燃烧指数 (GWFI) 960 °C IEC 60695-2-12
GWFI - 测试用试样厚度 2 mm -
电性能价值单位Test Standard
ISO数据
介质损耗因子, 1MHz 40 E-4 IEC 62631-2-1
体积电阻率 1E14 Ohm*m IEC 62631-3-1
介电强度 24 kV/mm IEC 60243-1
相对漏电起痕指数 150 - IEC 60112
其它性能价值单位Test Standard
吸水性 0.45 % 类似ISO 62
密度 1300 kg/m³ ISO 1183
加工推荐(注塑)价值单位Test Standard
预干燥-温度 120 - 150 °C -
预干燥-时间 3 - 5 h -
加工湿度 ≤0.02 % -
模具温度 170 - 200 °C -
加料温度 ≤100 °C -
1区 355 °C -
2区 360 °C -
3区 365 °C -
4区 370 °C -
喷嘴温度 375 °C -
典型数据
加工方法
注塑, 其它挤出成型
供货形式
粒料, 黑色
特殊性能
消毒
特征
脆性
耐化学试剂
通用耐化学性
Certifications
可食品接触的, FDA 21 CFR认证
应用
药物
地区供应
北美, 欧洲, 亚太, 中南美洲, 中东/非洲
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.